{"id":8709,"date":"2026-08-05T16:13:55","date_gmt":"2026-08-05T08:13:55","guid":{"rendered":"https:\/\/www.endlesswiresaw.com\/?p=8709"},"modified":"2026-08-05T16:15:35","modified_gmt":"2026-08-05T08:15:35","slug":"graphite-susceptor-ring-cutting","status":"publish","type":"post","link":"https:\/\/www.endlesswiresaw.com\/tr\/graphite-susceptor-ring-cutting\/","title":{"rendered":"Y\u00fcksek Safl\u0131kta Grafit S\u00fcspansiyon Halkas\u0131n\u0131 Kesme: \u00c7oklu Hassas Yuvalar, S\u0131f\u0131r Kenar \u00c7iplenmesi"},"content":{"rendered":"<p class=\"wp-block-paragraph\">B\u00fcy\u00fck \u00e7apl\u0131 bir grafit halka. \u00c7oklu hassas yuvalar. 40\u201370 m\/s h\u0131zda kuru kesim \u2014 ve her yuva duvar\u0131n\u0131n temiz \u00e7\u0131kmas\u0131 gerekiyor.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Grafit h\u0131zl\u0131 kesilir. Sorun bu de\u011fil. Sorun, grafittenin ayn\u0131 zamanda h\u0131zl\u0131 \u00e7atlamas\u0131 ve \u00e7ok yuval\u0131 b\u00fcy\u00fck silindirik bir halkada her kesim ge\u00e7i\u015finin, \u00e7atla\u011f\u0131n g\u00f6vde boyunca yay\u0131lmas\u0131 i\u00e7in ba\u015fka bir f\u0131rsat olmas\u0131d\u0131r. Bir yontulmu\u015f yuva duvar\u0131, bu noktaya kadar saatler s\u00fcren i\u015fleme tabi tutulmu\u015f t\u00fcm bile\u015fenin hurdaya \u00e7\u0131kmas\u0131 anlam\u0131na gelir.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Buna \u015fu \u015fekilde yakla\u015ft\u0131k.<\/p>\n\n\n\n<figure class=\"wp-block-image size-large\"><img fetchpriority=\"high\" decoding=\"async\" width=\"1024\" height=\"576\" src=\"https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/08\/graphite-susceptor-ring-cutting-sh60-60-1024x576.jpg\" alt=\"Vimfun Elmas Tel Testere Makinesi\" class=\"wp-image-8710\" title=\"Endless elmas tel testere makinesi, hassas kesim i\u00e7in m\u00fckemmel bir makine aletidir\" srcset=\"https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/08\/graphite-susceptor-ring-cutting-sh60-60-1024x576.jpg 1024w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/08\/graphite-susceptor-ring-cutting-sh60-60-300x169.jpg 300w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/08\/graphite-susceptor-ring-cutting-sh60-60-768x432.jpg 768w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/08\/graphite-susceptor-ring-cutting-sh60-60-1536x864.jpg 1536w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/08\/graphite-susceptor-ring-cutting-sh60-60-18x10.jpg 18w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/08\/graphite-susceptor-ring-cutting-sh60-60-600x338.jpg 600w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/08\/graphite-susceptor-ring-cutting-sh60-60.jpg 1672w\" sizes=\"(max-width: 1024px) 100vw, 1024px\" \/><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">Bile\u015fen: Yar\u0131 \u0130letken Termal \u0130\u015flemede Grafit S\u00fcspansiyon Halkalar\u0131<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">S\u00fcspansiyon halkalar\u0131, kristal b\u00fcy\u00fcme reakt\u00f6rleri ve y\u00fcksek s\u0131cakl\u0131kta wafer i\u015fleme ekipmanlar\u0131n\u0131n i\u00e7inde yer al\u0131r. G\u00f6revleri, termal i\u015flem s\u0131ras\u0131nda \u2014 1000\u00b0C \u00fczerindeki s\u0131cakl\u0131klarda \u2014 alt tabakalar\u0131 konumlar\u0131nda tutmakt\u0131r, bu s\u0131rada yuva geometrileri gaz ak\u0131\u015f\u0131n\u0131 ve \u0131s\u0131 da\u011f\u0131l\u0131m\u0131n\u0131 bile\u015fen y\u00fczeyi boyunca y\u00f6netir.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Y\u00fcksek safl\u0131kta <a href=\"\/graphite-cutting-machine\/\">grafit<\/a> bu uygulama i\u00e7in standart malzemedir. Tekrarlanan termal d\u00f6ng\u00fclere dayan\u0131r, reaktif proses gazlar\u0131na diren\u00e7 g\u00f6sterir ve karma\u015f\u0131k yuva profillerini tutacak kadar i\u015flenebilirli\u011fe sahiptir. Safl\u0131k spesifikasyonu kat\u0131d\u0131r: s\u00fcspansiyondan kaynaklanan eser metal kirlili\u011fi do\u011frudan wafer y\u00fczeyine aktar\u0131l\u0131r, bu nedenle yar\u0131 iletken s\u0131n\u0131f\u0131 grafit ,991 karbon veya daha y\u00fcksek oranda \u00e7al\u0131\u015f\u0131r.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Bu kombinasyon \u2014 termal olarak kararl\u0131, kimyasal olarak inert, y\u00fcksek safl\u0131kta \u2014 kirlenme riski veya yap\u0131sal hasar olmadan i\u015flenmesini zorla\u015ft\u0131ran tam olarak budur. Hizmette bozulmaya direnen malzeme, kesilmeye de diren\u00e7 g\u00f6sterir.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Sorun: K\u0131r\u0131lgan Grafitteki Yuvalar Darbeyi Affetmez<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Grafitin Mohs sertli\u011fi yakla\u015f\u0131k 1\u20132'dir. Kolayca kesilir. Yapmad\u0131\u011f\u0131 \u015fey darbeyi emmektir. Geleneksel bir frezeleme kesicisi veya testere b\u0131\u00e7a\u011f\u0131, kesme kuvvetini darbeler halinde uygular \u2014 her di\u015f temas\u0131, grafit tanecik yap\u0131s\u0131na mikro darbedir.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">K\u00fc\u00e7\u00fck bir grafit par\u00e7ada, bu darbeler genellikle y\u00f6netilebilir. \u00c7ok yuval\u0131 b\u00fcy\u00fck bir s\u00fcspansiyon halkas\u0131nda, \u00fc\u00e7 \u015fey sorunu art\u0131r\u0131r:<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Titre\u015fim seyahat mesafesi halka boyutuyla artar.<\/strong> Bir ucu kesici temas ederken di\u011fer ucu tutulan b\u00fcy\u00fck silindirik bir halka, bir kald\u0131ra\u00e7 g\u00f6revi g\u00f6r\u00fcr. Her di\u015f darbesinden kaynaklanan titre\u015fim, halka g\u00f6vdesi boyunca yay\u0131l\u0131r. Yuva duvarlar\u0131nda \u2014 kesitin en ince oldu\u011fu yerde \u2014 bu titre\u015fim, kenar yontulmas\u0131 veya y\u00fczey alt\u0131 \u00e7atlamas\u0131 olarak ortaya \u00e7\u0131kar.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Yuva say\u0131s\u0131 riski art\u0131r\u0131r.<\/strong> Kesilen her yuva, \u00f6nceki kesimlerden zaten gerilmi\u015f bir yap\u0131ya uygulanan ba\u015fka bir darbe olay\u0131d\u0131r. \u0130lk yuvay\u0131 hasars\u0131z ge\u00e7en bir halka, biriken mikro hasar bir e\u015fi\u011fe ula\u015ft\u0131\u011f\u0131nda d\u00f6rd\u00fcnc\u00fc veya be\u015finci ge\u00e7i\u015fte hala \u00e7atlama geli\u015ftirebilir. Bu nedenle, geleneksel testere ile \u00e7ok yuval\u0131 grafit halkalarda verim kayb\u0131, istisna olmaktan \u00e7ok verilmi\u015f kabul edilir.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Kertik kayb\u0131 termal dengeyi bozar.<\/strong> S\u00fcspansiyon halkas\u0131 yuva geometrisi, termal tasar\u0131m\u0131n bir par\u00e7as\u0131d\u0131r \u2014 yuva geni\u015fli\u011fi ve konumu, i\u015flem s\u0131ras\u0131nda \u0131s\u0131n\u0131n halka y\u00fczeyine nas\u0131l da\u011f\u0131ld\u0131\u011f\u0131n\u0131 belirler. Geni\u015f kertikli bir kesme y\u00f6ntemi, \u00e7izimde belirtilenden daha fazla malzemeyi yuva ba\u015f\u0131na kald\u0131r\u0131r, bu da halkan\u0131n termal performans\u0131n\u0131 kayd\u0131r\u0131r. Buradaki kertik kontrol\u00fc sadece malzeme israf\u0131 ile ilgili de\u011fildir; bu bir proses spesifikasyonudur.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img decoding=\"async\" width=\"920\" height=\"688\" src=\"https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/04\/graphite-multi-slice.png\" alt=\"Vimfun Elmas Tel Testere Makinesi\" class=\"wp-image-8036\" title=\"Endless elmas tel testere makinesi, hassas kesim i\u00e7in m\u00fckemmel bir makine aletidir\" srcset=\"https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/04\/graphite-multi-slice.png 920w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/04\/graphite-multi-slice-300x224.png 300w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/04\/graphite-multi-slice-768x574.png 768w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/04\/graphite-multi-slice-16x12.png 16w, https:\/\/www.endlesswiresaw.com\/wp-content\/uploads\/2026\/04\/graphite-multi-slice-600x449.png 600w\" sizes=\"(max-width: 920px) 100vw, 920px\" \/><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">Yakla\u015f\u0131m: SH60-60, 0,8 mm Tel, Kuru Kesim<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">kulland\u0131k <a href=\"https:\/\/www.endlesswiresaw.com\/products\/\" target=\"_blank\" rel=\"noreferrer noopener\">VIMFUN SH60-60<\/a> sonsuz elmas tel testere, 0,8 mm elektro kaplamal\u0131 <a href=\"\/diamond-wire-loops\/\">elmas tel d\u00f6ng\u00fcs\u00fc<\/a>.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><thead><tr><th>Parametre<\/th><th>De\u011fer<\/th><\/tr><\/thead><tbody><tr><td>Makine<\/td><td>VIMFUN SH60-60 Sonsuz Elmas Tel Testere<\/td><\/tr><tr><td>\u0130\u015f par\u00e7as\u0131<\/td><td>Y\u00fcksek safl\u0131kta grafit s\u00fcspansiyon halkas\u0131<\/td><\/tr><tr><td>Tel tipi<\/td><td>Elektro kaplamal\u0131 sonsuz elmas tel d\u00f6ng\u00fcs\u00fc<\/td><\/tr><tr><td>Tel \u00e7ap\u0131<\/td><td>0,8 mm<\/td><\/tr><tr><td>Kertik kayb\u0131<\/td><td>yuva ba\u015f\u0131na ~0,9 mm<\/td><\/tr><tr><td>Tel gerginli\u011fi<\/td><td>200\u2013300 N<\/td><\/tr><tr><td>Tel h\u0131z\u0131<\/td><td>40\u201370 m\/s<\/td><\/tr><tr><td>\u0130lerleme h\u0131z\u0131<\/td><td>50\u2013100 mm\/dak<\/td><\/tr><tr><td>So\u011futucu<\/td><td>Kuru kesim \u2014 so\u011futucu yok<\/td><\/tr><tr><td>Yuva geometrisi<\/td><td>\u00c7oklu radyal hassas yuvalar<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Grafit kuru kesilir. So\u011futucu yok. Grafit tala\u015f\u0131 reaktif de\u011fildir ve y\u00fcksek h\u0131zda telin kendi hava ak\u0131\u015f\u0131 alt\u0131nda kertikten \u00e7\u0131kar \u2014 so\u011futucu, yuvan\u0131n i\u00e7ine dolacak ve kesme direncini azaltmak yerine art\u0131racak bir grafit bulamac\u0131 olu\u015fturacakt\u0131r. Kuru kesim ayr\u0131ca, bir yar\u0131 iletken termal ortama giren bir bile\u015fen \u00fczerindeki so\u011futucu kal\u0131nt\u0131s\u0131ndan kaynaklanan kirlenme riskini de ortadan kald\u0131r\u0131r.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Tel h\u0131z\u0131 40\u201370 m\/s'de \u00e7al\u0131\u015f\u0131r \u2014 seramik veya kuvars gibi daha sert malzemelere g\u00f6re h\u0131zl\u0131d\u0131r ve daha kontroll\u00fc temas gerektirir. Grafittenin d\u00fc\u015f\u00fck sertli\u011fi, bu h\u0131zlarda malzeme kald\u0131rma oran\u0131n\u0131n y\u00fcksek oldu\u011fu ve a\u015f\u0131nd\u0131r\u0131c\u0131 etkinin tala\u015f temizli\u011fini ikincil bir y\u0131kama olmadan tutacak kadar agresif oldu\u011fu anlam\u0131na gelir. H\u0131z, gerilim ve beslemenin nas\u0131l etkile\u015fimde bulundu\u011funa dair daha fazla bilgi i\u00e7in bkz. <a href=\"\/wire-speed-tension-feed-rate\/\">Tel h\u0131z\u0131, gerginli\u011fi ve ilerleme h\u0131z\u0131<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">0,8 mm tel \u00e7ap\u0131, kertik yakla\u015f\u0131k 0,9 mm olarak ayarlan\u0131r. Bu, bu halka geometrisi i\u00e7in kas\u0131tl\u0131 bir se\u00e7imdir. Daha ince bir tel (0,4\u20130,6 mm) kertik daralt\u0131r ancak b\u00fcy\u00fck bir halkada birden fazla yuva ge\u00e7i\u015finde d\u00f6ng\u00fc yorulma riski olu\u015fturur \u2014 bu \u00e7aptaki yuva ba\u015f\u0131na uzat\u0131lm\u0131\u015f kesme yolu, t\u00fcm yuvalar tamamlanmadan \u00f6nce ince bir teli yorulma s\u0131n\u0131r\u0131na do\u011fru iter. 0,8 mm tel, t\u00fcm ge\u00e7i\u015flerde biraz daha geni\u015f bir kertik kar\u015f\u0131l\u0131\u011f\u0131nda tutarl\u0131 d\u00f6ng\u00fc b\u00fct\u00fcnl\u00fc\u011f\u00fc sunar.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Kritik parametre gerilim kontrol\u00fcd\u00fcr. 200\u2013300 N'deki tel gerilimi, her yuvan\u0131n tam derinli\u011fi boyunca sabit kalmal\u0131d\u0131r. Gerilim kesme s\u0131ras\u0131nda d\u00fc\u015ferse \u2014 servo avlanma, kasnak s\u00fcrt\u00fcnmesi veya yava\u015f tepki veren bir gerilim d\u00f6ng\u00fcs\u00fc nedeniyle \u2014 tel yanal olarak yaylan\u0131r ve yuva duvar\u0131 konik olarak \u00e7\u0131kar: giri\u015fte \u00e7\u0131k\u0131\u015ftan daha geni\u015f. SH60-60\u2019\u0131n kapal\u0131 d\u00f6ng\u00fc gerilim sistemi sapmalar\u0131 ger\u00e7ek zamanl\u0131 olarak d\u00fczeltir. Tutarl\u0131 gerilim, halkadaki her yuva boyunca paralel yuva duvarlar\u0131 \u00fcretir.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Sonu\u00e7: Her Yuva Duvar\u0131 Temiz, \u0130kincil \u0130\u015flem Yok<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Kesimden sonra, her yuva hem giri\u015fte hem de \u00e7\u0131k\u0131\u015fta temiz kenarlar g\u00f6sterir \u2014 yontulma yok, duvarlarda mikro \u00e7atlak yok, \u00e7\u0131k\u0131\u015f taraf\u0131nda delaminasyon yok.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Yuva geometrisi t\u00fcm kesimlerde tutarl\u0131d\u0131r. Tekd\u00fcze geni\u015flik, paralel duvarlar, d\u00fcz yuva taban\u0131. Kesme de\u011fi\u015fkeninin \u2014 tel konumu, gerilimi, h\u0131z\u0131 \u2014 ilk yuva ile son yuva aras\u0131nda kaymad\u0131\u011f\u0131 bir s\u00fcre\u00e7ten gelen tutarl\u0131l\u0131k t\u00fcr\u00fc.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Olmayanlar, olanlar kadar \u00f6nemlidir. Geleneksel i\u015fleme y\u00f6ntemlerinde, halka hizmete girmeden \u00f6nce yontulmu\u015f grafit par\u00e7ac\u0131klar\u0131n\u0131 temizlemek i\u00e7in yuva kesimini genellikle bir \u00e7apak alma i\u015flemi takip eder. Bir yar\u0131 iletken termal ortam\u0131ndaki grafit tala\u015flar\u0131 s\u00fcreci kirletir. Bu ad\u0131m\u0131 atlamak sadece bir verimlilik art\u0131\u015f\u0131 de\u011fildir - ayn\u0131 zamanda \u00e7apaklanma riski getiren bir elle\u00e7leme a\u015famas\u0131n\u0131 ortadan kald\u0131r\u0131r. Elmas tel i\u015flemi, buna ihtiya\u00e7 duymayan yuva duvarlar\u0131 sa\u011flar. Elmas tel kesiminde y\u00fczey sonucu kontrol\u00fc hakk\u0131nda ayr\u0131nt\u0131l\u0131 bilgi i\u00e7in bkz. <a href=\"\/surface-quality-optimization\/\">y\u00fczey kalitesi optimizasyonu<\/a>.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Yuva duvarlar\u0131ndaki y\u00fczey alt\u0131 \u00e7atlak durumu da geleneksel kesimin geride b\u0131rakt\u0131\u011f\u0131ndan farkl\u0131d\u0131r. Y\u00fczey \u00e7apaklanmas\u0131 g\u00f6r\u00fcn\u00fcrd\u00fcr ve muayenede derecelendirilebilir. Y\u00fczey alt\u0131 \u00e7atlaklar g\u00f6r\u00fcnmezdir ancak termal d\u00f6ng\u00fcler s\u0131ras\u0131nda yay\u0131l\u0131r - s\u00fcre\u00e7 ortas\u0131nda bile\u015fen ar\u0131zas\u0131na yol a\u00e7ar. Sonsuz elmas telin d\u00fc\u015f\u00fck etkili a\u015f\u0131nd\u0131rma mekanizmas\u0131, vurmal\u0131 kesimin getirdi\u011fi \u00e7atlak ba\u015flatma derinli\u011fi olmadan y\u00fczey alt\u0131 hasar\u0131n\u0131 yaln\u0131zca a\u015f\u0131nd\u0131rma b\u00f6lgesiyle s\u0131n\u0131rlar. <a href=\"https:\/\/www.sglcarbon.com\/en\/markets-and-solutions\/semiconductors\/\" target=\"_blank\" rel=\"noreferrer noopener\">SGL Carbon'un yar\u0131 iletken uygulamalar\u0131 i\u00e7in y\u00fcksek safl\u0131kta grafit k\u0131lavuzuna g\u00f6re<\/a>, termal d\u00f6ng\u00fcler boyunca boyutsal kararl\u0131l\u0131k, i\u015fleme a\u015famas\u0131ndan itibaren \u00e7atlaks\u0131z bir durumla ba\u015flar.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Halka, yar\u0131 iletken termal i\u015fleme ekipmanlar\u0131 i\u00e7in makineden haz\u0131r olarak \u00e7\u0131kar. \u0130kincil kenar i\u015fleme yok. So\u011futucu kal\u0131nt\u0131s\u0131ndan kaynaklanan kirlenme riski yok. T\u00fcm ge\u00e7i\u015flerde spesifikasyon dahilinde yuva geometrisi.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"https:\/\/www.spiedigitallibrary.org\/conference-proceedings-of-spie\" target=\"_blank\" rel=\"noreferrer noopener\">SPIE bildirileri, yar\u0131 iletken termal uygulamalar i\u00e7in grafit i\u015fleme \u00fczerine<\/a> k\u0131r\u0131lgan grafit bile\u015fenlerde elmas tel ve geleneksel i\u015fleme aras\u0131ndaki y\u00fczey durumu fark\u0131n\u0131 belgelemektedir - bu fark, bile\u015fen karma\u015f\u0131kl\u0131\u011f\u0131 artt\u0131k\u00e7a b\u00fcy\u00fcr.<\/p>\n\n\n\n<figure class=\"wp-block-embed is-type-video is-provider-youtube wp-block-embed-youtube wp-embed-aspect-16-9 wp-has-aspect-ratio\"><div class=\"wp-block-embed__wrapper\">\n<div  id=\"_ytid_27172\"  width=\"640\" height=\"360\"  data-origwidth=\"640\" data-origheight=\"360\" data-facadesrc=\"https:\/\/www.youtube.com\/embed\/zw0KQkAbSD4?enablejsapi=1&#038;autoplay=0&#038;cc_load_policy=0&#038;cc_lang_pref=&#038;iv_load_policy=1&#038;loop=0&#038;rel=1&#038;fs=1&#038;playsinline=0&#038;autohide=2&#038;theme=dark&#038;color=red&#038;controls=1&#038;disablekb=0&#038;\" class=\"__youtube_prefs__ epyt-facade epyt-is-override  no-lazyload\"><img decoding=\"async\" data-spai-excluded=\"true\" class=\"epyt-facade-poster skip-lazy\" loading=\"lazy\" alt=\"YouTube oynat\u0131c\u0131\" src=\"https:\/\/i.ytimg.com\/vi\/zw0KQkAbSD4\/maxresdefault.jpg\" title=\"Endless elmas tel testere makinesi, hassas kesim i\u00e7in m\u00fckemmel bir makine aletidir\"><button class=\"epyt-facade-play\" aria-label=\"Oynat\"><svg data-no-lazy=\"1\" height=\"100%\" version=\"1.1\" viewbox=\"0 0 68 48\" width=\"100%\"><path class=\"ytp-large-play-button-bg\" d=\"M66.52,7.74c-0.78-2.93-2.49-5.41-5.42-6.19C55.79,.13,34,0,34,0S12.21,.13,6.9,1.55 C3.97,2.33,2.27,4.81,1.48,7.74C0.06,13.05,0,24,0,24s0.06,10.95,1.48,16.26c0.78,2.93,2.49,5.41,5.42,6.19 C12.21,47.87,34,48,34,48s21.79-0.13,27.1-1.55c2.93-0.78,4.64-3.26,5.42-6.19C67.94,34.95,68,24,68,24S67.94,13.05,66.52,7.74z\" fill=\"#f00\"><\/path><path d=\"M 45,24 27,14 27,34\" fill=\"#fff\"><\/path><\/svg><\/button><\/div>\n<\/div><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">Grafit Y\u00fcksek S\u0131cakl\u0131k Halka Kesebilir miyiz?<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Grafit halka \u0131s\u0131t\u0131c\u0131lar, CZ pota astarlar\u0131, \u0131s\u0131tma elemanlar\u0131 ve di\u011fer karma\u015f\u0131k grafit termal alan bile\u015fenlerini i\u015fliyoruz.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">\u00c7e\u015fitli geometrilerde bo\u015fluklar, paneller ve yap\u0131sal lamine b\u00f6l\u00fcmler i\u00e7in GFRP elmas tel kesimi sa\u011fl\u0131yoruz. Kal\u0131n b\u00f6l\u00fcmlerde delaminasyon, sa\u00e7\u0131lm\u0131\u015f \u00e7\u0131k\u0131\u015f kenarlar\u0131 veya geleneksel testerelerin kar\u015f\u0131lamad\u0131\u011f\u0131 toz kontrol gereksinimleriyle u\u011fra\u015f\u0131yorsan\u0131z, burada a\u00e7\u0131klanan SH60-60 s\u00fcreci pratik bir ba\u015flang\u0131\u00e7 noktas\u0131d\u0131r.<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li>Halka d\u0131\u015f \u00e7ap\u0131 ve i\u00e7 \u00e7ap\u0131<\/li>\n\n\n\n<li>Et kal\u0131nl\u0131\u011f\u0131 ve yuva say\u0131s\u0131<\/li>\n\n\n\n<li>Yuva geni\u015fli\u011fi hedefi ve yuva derinli\u011fi<\/li>\n\n\n\n<li>Grafit kalitesi (safl\u0131k, tane yap\u0131s\u0131) biliniyorsa<\/li>\n\n\n\n<li>Kenar kalitesi gereksinimi veya mevcut \u00e7izim toleranslar\u0131<\/li>\n<\/ul>\n\n\n\n<p class=\"wp-block-paragraph\">SH60-60'\u0131n geometrinize uyup uymayaca\u011f\u0131n\u0131 teyit edecek, yuva profiliniz i\u00e7in tel \u00e7ap\u0131 ve parametreleri belirtecek ve halka boyutunuz i\u00e7in fikst\u00fcrleme konusunda tavsiyede bulunaca\u011f\u0131z.<\/p>","protected":false},"excerpt":{"rendered":"<p>A large-diameter graphite ring. Multiple precision slots. Dry-cut at 40\u201370 m\/s \u2014 and every slot wall has to come out clean. Graphite cuts fast. That&#8217;s not the problem. The problem is that graphite also fractures fast, and on a large cylindrical ring with multiple slots, each cut pass is another opportunity for a crack to [&hellip;]<\/p>\n","protected":false},"author":6,"featured_media":8710,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"set","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[452],"tags":[979,1105,1106],"class_list":["post-8709","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-technical-insights","tag-case-study","tag-graphite-cutting","tag-semiconductor-thermal-components"],"acf":[],"_links":{"self":[{"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/posts\/8709","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/users\/6"}],"replies":[{"embeddable":true,"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/comments?post=8709"}],"version-history":[{"count":2,"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/posts\/8709\/revisions"}],"predecessor-version":[{"id":8712,"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/posts\/8709\/revisions\/8712"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/media\/8710"}],"wp:attachment":[{"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/media?parent=8709"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/categories?post=8709"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.endlesswiresaw.com\/tr\/wp-json\/wp\/v2\/tags?post=8709"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}